1/16" Balsa

Collapse
X
 
  • Time
  • Show
Clear All
new posts
  • Royatl
    In Memoriam
    • Mar 2005
    • 2646
    • Atlanta, GA

    #16
    Originally posted by tbzep
    Next time you guys use 1/16" balsa for large fins, don't use thinned F-n-F to fill the grain. I made it thick as I could and still brush it on and it still warped the fins. I got them straight after the first application and I will after this one, but it is a pain in the butt to fool with. Just thought I'd vent a bit.
    I use it on 1/16" balsa all the time.

    before... Choose hard C-grain balsa if possible. A-grain is just asking for trouble anyway.
    1. apply it BEFORE attaching to rocket
    2. use it full strength and apply it with your finger (vinyl or nitrile glove recommended). rub it in.
    3. apply it on both sides at roughly the same time (i.e. not one side and let dry, then other side)


    from what I can tell in the picture, your fins were close to A-grain, and your F'n'F had a much higher water content than it needed to be.
    Roy
    nar12605

    Comment

    • SecretSquirrel
      Craftsman
      • Nov 2008
      • 268

      #17
      Originally posted by Doug Sams
      I imagine the density was a key factor. It likely limited the absorption and thus minimized the warping.

      I rarely use 1/16" preferring to instead upgrade most of my clones to 3/32" for the sake of durability. That said, I still use it on occasion and don't see many problems. I normally lay down a coat of Zinnser primer first, and I wonder if that averts the warping by limiting the absorption of the thinned FnF.

      Doug...thinking out loud...

      .

      Could be, I usually brush on a coat of clear dope to limit absorption and it seems to work fairly well.
      Don Magness
      http://www.squirrel-works.com/

      Follow us on Facebook

      Even the best of friends cannot attend each others' funeral.

      Comment

      • scigs30
        Master Modeler
        • Jul 2006
        • 2462

        #18
        I am finishing my Apogee II right now and it is an original so I used the balsa stock that came with the kit. I used Aerogloss balsa sealer, 4 coats and no warps. After 1 coat of grey primer the grain was all filled. Since I am building the original, I don't have the luxury of using basswood.

        Comment

        • Mark II
          Forest Sprite
          • Dec 2006
          • 3657
          • Back Up in the Woods

          #19
          I still mostly use balsa, but I pick the sheets with the hardest C-grain that I can find. I also use basswood on occasion, especially on larger rockets, but I'm thinking about using it more often. Thick basswood, like 1/4" or thicker, is A LOT of work to sand. (I use a a palm sander, and even then, it takes awhile.) Yeah, basswood is more forgiving than balsa to sand, in a sense, but that is because you have to make many, many more strokes (and go through much more sandpaper) to remove the same amount of stock. When you are making, say, 200 or more strokes to round one edge of a fin, as opposed to, say, making 30, it is easier to make subtle adjustments to correct minor errors.

          I have used this stuff (see attached image) to fill the grain in balsa fins, and I have not seen any warping. Once the Delta Ceramcoat filler is completely dry, you can give it a light wet-sanding with 400-grit sandpaper to get a nice smooth surface. It may require 2-3 coats, depending on how coarse the grain is. I also use it on nose cones. You can find it in the crafts section at Walmart, and at Joanne's Fabrics and Michael's.

          One other filler that has worked well for me is Pine-Pro Sanding Sealer, which I have only seen at my local hobby shop (in with the pinecar derby supplies), but you might be able to find it at Michael's, too. It is thicker and it fills faster than the Delta product, and it also wet-sands smoother. Unfortunately, I can only find it in small bottles, and it goes fast. (I used almost an entire 2 oz. bottle on my Golden Scout. ) Because of that, I mainly just use it on nose cones. But this stuff is truly great, and it is what I would use all the time, if I could get it in larger bottles. The Delta Ceramcoat filler and Pine-Pro are both water-based, but I have never had either one cause fin warping. They both just clean off my brushes with soap and water. Before you wet-sand either one, though, make sure that the coat has completely dried.



          Mark \\.
          Attached Files
          Mark S. Kulka NAR #86134 L1,_ASTRE #471_Adirondack Mountains, NY
          Opinions Unfettered by Logic • Advice Unsullied by Erudition • Rocketry Without Pity
          +09281962-TAK-08272007+
          SAM # 0011

          Comment

          • Mark II
            Forest Sprite
            • Dec 2006
            • 3657
            • Back Up in the Woods

            #20
            BTW, I also think that FSI might have been on to something when they used 1/16" aircraft plywood for the fins in many of their kits. It is very hard, and if the fins aren't too big, there isn't much of a weight penalty. Tack the stuff on with gel CA, then give it some thin epoxy fillets, and the fins are bullet-proof! The birch aircraft ply that I have used was finished much smoother than regular plywood. It still needed to be sealed, but it usually just needed one light coat of filler to completely fill the grain. The downside? It was almost as hard to sand as basswood (almost) . I haven't tried make fins from 1/32" birch plywood yet, but it might work out that the slight extra weight would be offset by the much thinner aerodynamic cross-section.

            Mark \\.
            Mark S. Kulka NAR #86134 L1,_ASTRE #471_Adirondack Mountains, NY
            Opinions Unfettered by Logic • Advice Unsullied by Erudition • Rocketry Without Pity
            +09281962-TAK-08272007+
            SAM # 0011

            Comment

            • MKP
              Craftsman
              • Aug 2007
              • 222
              • High Desert of Utah

              #21
              I also use the Delta Cream Coat, and really like it. I've tried both it and Aerogloss, and the Delta product seems to work just as well and isn't nearly as toxic and stinky. (When I use Aerogloss everyone in the house gives me grief.)
              "Men and steel are alike. When they lose their temper they lose their worth." - Chuck Norris

              Comment

              • micromeister
                Micro Builder
                • Sep 2007
                • 60
                • Washington D.C.

                #22
                Seems that 3 coats are the Charm regardless of the "filler material" being used.

                Sigs30 used sanding sealer, some use (myself included) have or are using Balsa filler containing much higher solids, other are using waterbased sealer/fillers.
                I've all but stopped using these "fillers" long ago.

                Since i'm going to be priming and sanding the model anyway thats were i've learned to start.
                Indstead of wasting a bunch of time with fillers I Start with whatever el-cheap-O rattle can primer I can find on the raw wood and bodytubes. As with all the other methods... open grain balsa fins, cones and transitions generally takes 3 coats to fill the grain. Basswood I've found can generally get away with two coats. DRY sand with 120 to 320girt papers to a babies but smooth surface ready for whatever base or color I choose. Recently I've been using a Walmart .89 grey auto primer with excellant results under Krylon (old formula) and rustoleum color coats .

                Drawbacks: * Sometimes takes an entire can to fill a large model (like the E-interceptor).
                *Should use a spraybooth or box to contain a bit of overspary.
                * if spraying indoors you'll want to exhaust the smell outside with a blower.

                Advantages: * Less smell than Pactra or other brand Lacquer based fillers.
                * No brushing or trowel applying messy fillers.
                * Much Quicker filling.
                * generally less expensive (depending on primer used).
                * Fills Bodytube seams and grain at the same time.
                * Fewer steps to the completed model.
                Hope this helps.
                Keep em flyin Micronized
                John

                Comment

                • tbzep
                  Dazed and Confused
                  • Mar 2005
                  • 12833
                  • TN

                  #23
                  Originally posted by micromeister
                  Drawbacks: * Sometimes takes an entire can to fill a large model (like the E-interceptor).
                  *Should use a spraybooth or box to contain a bit of overspary.
                  * if spraying indoors you'll want to exhaust the smell outside with a blower.
                  Those reasons are part of why I use Fill-n-Finish. The biggest reason is that I can sand the stuff in 10 minutes. The only primer that comes that close is lacquer primer, and the only lacquer I can get here is very expensive, so I only use it after slicking up all the balsa with F-n-F.

                  I hate sanding, so when I finally get in the mood, I need to get on it quick and get it over with.
                  I love sanding.

                  Comment

                  • cas2047
                    Master Modeler
                    • Jun 2006
                    • 1532
                    • MA, NH

                    #24
                    Originally posted by tbzep
                    I hate sanding, so when I finally get in the mood, I need to get on it quick and get it over with.
                    I'm with you there.

                    How will you, or how did you fix the warped fin? It looks like it would need to be sanded, wet down and clamped in between two flat pieces of wood or metal...
                    I plan ahead that way I don't have to do anything right now.

                    Oh by the way, I'm not here just for the "olde" rocket discussions.

                    Comment

                    • Mark II
                      Forest Sprite
                      • Dec 2006
                      • 3657
                      • Back Up in the Woods

                      #25
                      I can't argue with your results, Micromeister, but I'm a bit squeamish about sanding raw balsa nose cones, even if they have a coat or two of primer on them. I used to do that, but too many times I ended up with misshaped nose cones!

                      Your method is exactly what I used to do when I started building rockets again a few years ago. Eventually I started using fillers and sealers before priming because they gave me much better results!

                      A bottle of Delta Ceramcoat All-Purpose Sealer also lasts a whole lot longer than many cans of spray primer. Two years ago, I bought two 8 oz. bottles of it at Walmart. I'm still on the first bottle.

                      I do agree that the extra steps are a bit of a pain, though. I'm always in favor of finding, simpler, easier methods to accomplish the same thing.

                      Also, as I mentioned in a thread awhile ago on finishing techniques (or was it on Krylon paint?), I suspect that what methods work best for an individual builder may depend, in part, on what part of the country (or world) that he or she lives in, and what the predominant climate is like in the area. I don't know that this is true, but I suspect that it might play some role.

                      I do all of my spraying outdoors and out in the open on warm, dry days when there is little or no wind. (Where I live, that limits me to doing all of my painting during a few weeks in high summer.) To avoid blushing the paint, I do not do the spraying out in my yard, because the area over the grass, and in the vicinity of shrubs, etc., has higher humidity than elsewhere. I take my rockets down to the end of my driveway, or even out to the street in front of my house, to lay on coats of spray paint. The air is always drier in those places. (In addition to the general climate of a local area, there are little micro-climates over and around everything, especially living things like plant foliage.) If I had a large slab of concrete (not asphalt) to go to that was out in the sun for part of the day (and would therefore be well-dried) and that was free of dust and wind, that's where I would do all of my spray painting.

                      Or else a well-designed and well-ventilated spray booth...

                      Mark \\.
                      Last edited by Mark II; 12-17-2008, 12:40 PM.
                      Mark S. Kulka NAR #86134 L1,_ASTRE #471_Adirondack Mountains, NY
                      Opinions Unfettered by Logic • Advice Unsullied by Erudition • Rocketry Without Pity
                      +09281962-TAK-08272007+
                      SAM # 0011

                      Comment

                      • tbzep
                        Dazed and Confused
                        • Mar 2005
                        • 12833
                        • TN

                        #26
                        Originally posted by cas2047
                        I'm with you there.

                        How will you, or how did you fix the warped fin? It looks like it would need to be sanded, wet down and clamped in between two flat pieces of wood or metal...
                        I just moistened spots here and there and let it warp itself back straight on its own.
                        I love sanding.

                        Comment

                        • micromeister
                          Micro Builder
                          • Sep 2007
                          • 60
                          • Washington D.C.

                          #27
                          Originally posted by tbzep
                          Those reasons are part of why I use Fill-n-Finish. The biggest reason is that I can sand the stuff in 10 minutes. The only primer that comes that close is lacquer primer, and the only lacquer I can get here is very expensive, so I only use it after slicking up all the balsa with F-n-F.

                          I hate sanding, so when I finally get in the mood, I need to get on it quick and get it over with.

                          Absolutely with you there !!! I hate sanding as well. but if we're going to get a decent finish we have to bite the bullet and sand on something. I've just eliminated most of the in between stuff.
                          Depending on were you live and the humidity level at the time your priming one can be sanding in less then an hour. I usually try to let each of the three coats set up for about 5 to 10 minutes, then wait about a half hour after the 3rd coat is applied. If the primer starts building up to quickly on the papers, I let it set awhile longer, or even let it go overnight if the humidity is high in the house

                          I'm not sure I follow you Mark? sanding on RAW balsa??? it's got at least 3 heavy coats of sandable primer... Not hard as nails but at least as hard as balsa filler/ sanding sealer and surely harder then f-N-f.
                          I can't remember the last time I really screwed up a nosecone or transition during sanding. If you start to see wood ya just add another coat before continuing.
                          yeah! I guess i'm pretty lucky I live in a Very high humidity area but have outfitted the rocket lab with two spray booths so I can spary anytime I want.
                          I will give the Delta ceramcoat a try in the future, I'm always looking for products and techniques to update my Tech-tip articles series.
                          Keep em flyin Micronized
                          John

                          Comment

                          • Mark II
                            Forest Sprite
                            • Dec 2006
                            • 3657
                            • Back Up in the Woods

                            #28
                            Originally posted by micromeister
                            [...]
                            I'm not sure I follow you Mark? sanding on RAW balsa??? it's got at least 3 heavy coats of sandable primer... Not hard as nails but at least as hard as balsa filler/ sanding sealer and surely harder then f-N-f.
                            I can't remember the last time I really screwed up a nosecone or transition during sanding. If you start to see wood ya just add another coat before continuing.
                            yeah! I guess i'm pretty lucky I live in a Very high humidity area but have outfitted the rocket lab with two spray booths so I can spary anytime I want.
                            I will give the Delta ceramcoat a try in the future, I'm always looking for products and techniques to update my Tech-tip articles series.
                            OK, maybe I misunderstood - I thought that you were talking about sanding in between each of those first coats of primer. Also, were you talking about using high-build primer?

                            Maybe I have gotten gun-shy from my earlier experiences, but I am very reluctant to touch sandpaper to a nose cone until I have, at a minimum, sealed the surface. I want to be sure that I am just sanding the surface grain, and not the cone itself. It may just be me, but ever since I started taking that precaution, I haven't messed up any more nose cones.

                            When I sand the filler/sealer coat, I wet-sand with 400 to 600 grit sandpaper. I am not really sanding the stuff off, but rather, it is more like I am smoothing it out. I try whenever possible to use the approach of building up a smooth surface through the application of many thin layers, rather than flooding the surface of the object and then sanding it down to something smooth.

                            As for sanding in general, I don't mind it at all myself, as long as it is producing good results. I like the look of a smooth paint job better than a rough one, and so I will do the work that is needed to get that look. I get great satisfaction when I can see that the surface is looking better and better as I sand it. But I haven't shown very many of my builds to anyone else yet; the reason I put so much care into the finish of them is purely for personal satisfaction.

                            Mark \\.
                            Mark S. Kulka NAR #86134 L1,_ASTRE #471_Adirondack Mountains, NY
                            Opinions Unfettered by Logic • Advice Unsullied by Erudition • Rocketry Without Pity
                            +09281962-TAK-08272007+
                            SAM # 0011

                            Comment

                            • tbzep
                              Dazed and Confused
                              • Mar 2005
                              • 12833
                              • TN

                              #29
                              Originally posted by Mark II
                              Maybe I have gotten gun-shy from my earlier experiences, but I am very reluctant to touch sandpaper to a nose cone until I have, at a minimum, sealed the surface. I want to be sure that I am just sanding the surface grain, and not the cone itself. It may just be me, but ever since I started taking that precaution, I haven't messed up any more nose cones.
                              Use what works for you. That's the beauty of reading all the different methods and materials. It all ends up looking good in the end, but different techniques and materials work better for different folks.

                              One thing I haven't done, but have read about here and thought it had merit is to use a different color primer for the first coat so that you see when you are getting down near the wood. You could then use a different color primer over it, or Fill-n-Finish, or any other type of filler. That might be what you are doing when you use a sealer first.

                              There's one thing I have figured out over the years, and believe me, I've tried to prove it wrong. No matter what method or materials I use, I'm gonna have to do a lot of sanding to get a good looking finish.
                              I love sanding.

                              Comment

                              • scigs30
                                Master Modeler
                                • Jul 2006
                                • 2462

                                #30
                                I have experimented with Aerogloss sealer and filler. Multiple coats of primer no sealer. Ceramcote and FNF. I will agree they all worked but each had advantages and disadvantages. For me Aerogloss sealer fits my building style so that is what I use. Also all the above techniques still require proper application and sanding technique. If you are sloppy with sanding, well the finished product will look sloppy. With Aerogloss sealer, I am able to sand after 1/2 hour and 3 to 4 coats is plenty. I am using old balsa wood from vintage kits. I apply the sealer the same way I apply filler when building wood projects. I make a conscious effort to brush the sealer into the grain using a stiff brush. I noticed in the beginning when I just half hazardly brushed the sealer on, the grain would not fill. But now that I am using a stiffer brush the sealer makes it into the grain. So basically it is 2 coats of sealer, sand, one coat sand and possibly one last coat and sand. I sand with 320 to 400 gritt. If I was unable to use Aerogloss, I would probably use Ceramcote. There is no oder and clean up is easy. I did find it tougher to sand, almost like sanding Elmers glue.

                                Comment

                                Working...